【摘要】以某SUV车型流水槽后部为例,介绍了制件冲压成形工艺、模具结构,以及模具精
度调试过程中出现的起皱开裂等问题解决。通过冲压成形性模拟分析、机床设备、板料、
模具调试等方面综合分析车身流水槽件开裂起皱问题,提高尺寸精度和外观匹配质量,减
少模具调模时间,降低白车身整车AUDIT质量评价扣分,改变客户对汽车外观质量的感观
评价。
关键词:冲压件;模拟分析;整形;开裂;起皱;模具调试
中图分类号:TG385.2文献标识码:B
DOI:10.12147/jki.l671-350&2019.10.011汽车在线gps定位
Cause Analysis and Countermeasure of Cracking
and Wrinkle in Shaping Flume of SUV Vehicle Type [Abstract]Taking the rear part of a SUV running water tank as an example,the article introduces the stamping process,die structure,and the countermeasures to solve the wrinkling and cracking problems in the process of die precision restoration and debugging.Through simulation analysis of stamping formability,machine tool equipment,sheet metal,die
新胜达汽车debugging and other aspects,the cracking and wrinkling problems of the body running water tank are comprehensively analyzed to improve dimensional precision and appearance matching quality,reduce die adjustment time,reduce AUDIT quality evaluation deduction,and change customer's perception evaluation of automobile appearance quality.
Key words:stamping parts;simulation analysis;sizing;cracking;wrinkling;die debugging
1引言
汽车行业竞争日益激烈,MPV.SU V车型也越来越受欢迎,汽车消费者对车身外观质量的要求也越来
越高。目前SUV车型的后背门多数采用掀背式产品设计,整个后背尾门整体开启后,可以清楚地看到整个流水槽的外观造型结构,其外观视觉效果直接体现了汽车企业的设计和制造水平。本文介绍了SUV车型车身后流水槽本体工艺结构设计、模拟成形性分析、冲压设备、板料等方面阐述如何解决车身开启件起皱开裂的原因及解决对策研究。
5月新规2流水槽车身匹配搭接关系介绍
车身后背门流水槽主要是将车身雨水沿着制件导向槽排出车外,防止水流进入车身内部造成锈蚀,车身流水槽后部与侧围外板,流水槽上部、顶盖外板搭接焊接而成。因此对流水槽后部模具工艺排布、结构设计、制件尺寸符合率、外观质量要求极高,外观匹配质量要求外露面无起皱开裂等质量缺陷,在设计结构的同时,需要考虑外观匹配要求,保证良好的匹配,亮丽的整车美观,图1所示为流水槽车身匹配搭接关系和外观结构。iem4
3流水槽工艺结构分析
此制件结构型面复杂,成形难度大,拉伸成形较深,工艺排布复杂,车身流水槽下部板料材质为HC180Y,板料厚度0.7mm,制件尺寸243x225x